Tsarin Zazzabi na Nodular Cast Iron
Tsarin jiyya mai zafi: gaba ɗaya kashewa
Quenching: dumama a 875 ~ 925ºC zazzabi, riƙewa na 2 ~ 4h, kashewa cikin mai don samun tsarin matrix martensite
Zazzabi: zazzabi mai tsananin zafi a 550 ~ 600ºC don samun tsarin sihiri mai ɗaci + ƙaramin adadin ferrite + spheroidal graphite
350 ~ 500ºC tempering a matsakaici zafin jiki don samun zafin troostite tsarin + karamin adadin ferrite + spheroidal graphite
Mai zafi a 150 ~ 250ºC don samun tsarin martensite mai zafi + ƙaramin adadin ferrite + dutse mai siffar zobe.
Wasu: Manufar: don samun ƙarfi (> 700MPa), ƙarancin aikin elongation
lura:
- CanYana iya hana tsagewa kuma ana iya kashe shi zuwa 200ºC mai mai zafi;
- IsYana da kyau a daidaita al'ada kafin a kashe
Tsarin jiyya mai zafi: farfajiya da jiyya mai zafi
Quenching: harshen wuta ko shigar da dumama zai zafi saman simintin zuwa 850 ~ 950ºC, zurfin dumama zai iya kaiwa 2 ~ 4mm, kashe ruwa.
Zazzabi: 380 ~ 410ºC zafin zafin wutar makera
Wasu: Manufa: inganta taurin ƙasa da sa juriya, da samun madaurin martensite tare da taurin 600 ~ 700HV
Lura: Yi amfani da magani na al'ada kafin kashewa, pearlite> 70% (ƙaramin juzu'i)
Quenching: Nitriding a 550 ~ 600ºC, zurfin 0.1m
Tsarin jiyya mai zafi: Austempering
Quenching: babban zazzabi isothermal quenching: dumama zuwa 875 ~ 925ºC, riƙe don 2 ~ 4h, kashe a 400 ~ 450ºC gishiri wanka na 1 ~ 6h, sannan sanyaya zuwa zafin jiki
Wasu: Babban abin da aka samu shine tsarin babban bainite + mafi riƙe da austenite. Cast baƙin ƙarfe na iya samun babban tauri, babban ƙarfi da matsakaicin taurin, kuma yana da ƙwarewar aiki mai ƙarfi. Aikin sa shine babban tsawo da raunin karaya mai ƙarfi, wanda yakamata a danganta shi da riƙe austenite
Quenching: Ƙananan zafin jiki austempering: tsarin dumama iri ɗaya ne da na sama. Kashe a cikin wanka mai gishiri a 235 ~ 350ºC na 1 ~ 6h, sannan sanyaya zuwa zafin jiki
Wasu: Babban abin da aka samo shine ƙananan bainite + ɓangaren riƙe austenite. Yana da babban ƙarfi, wasu filastik da tauri, kuma yana da ikon yin taurin kai. Yana da juriya mafi girma fiye da sauran baƙin ƙarfe na ductile.
Da fatan za a adana tushe da adireshin wannan labarin don sake bugawa: Tsarin Zazzabi na Nodular Cast Iron
Minghe Kamfanin 'Yan Wasa Masu Mutu aka sadaukar domin tsirar da samar da inganci da kuma high yi Gyare sassa (karfe mutu simintin sassa Range yafi hada da Thin-Wall Mutu Wasa,Hot Chamber Mutu Wasa,Cold Chamber Mutu Wasa), Zagaye Sabis (Mutuwar 'Yan Wasa,CNC machining,Motsa Motsa, Jiyya na sama) .Adadin al'ada Aluminium ya mutu, magnesium ko Zamak / zinc mutu simintin gyare-gyare da sauran buƙatun simintin maraba don tuntube mu.
Karkashin kulawar ISO9001 da TS 16949, Ana aiwatar da dukkan matakai ta hanyar daruruwan injunan jefa simintin da suka mutu, injunan axis 5, da sauran kayan aiki, tun daga masu fashewa zuwa na’urar Ultra Sonic masu wanki.Minghe ba kawai tana da kayan aiki na zamani ba amma kuma tana da kwararru ƙungiyar ƙwararrun injiniyoyi, masu aiki da sufetoci don tabbatar da ƙirar abokin ciniki ta zama gaskiya.
Manufactureran kwangilar masana'antar mutu. Abubuwan haɓakawa sun haɗa da sassan sanyi na sassan mutuɗar aluminum daga 0.15 lbs. zuwa 6 lbs., saurin canje-canje da aka saita, da aikin inji. Sabis-ƙarin ayyuka sun haɗa da gogewa, faɗakarwa, lalatawa, fashewar harbi, zane, zane, rufi, haɗuwa, da kayan aiki. Abubuwan da aka yi aiki tare sun haɗa da allo irin su 360, 380, 383, da 413.
Zinc ya mutu don jefa ƙirar ƙira / sabis na injiniya tare. Custom manufacturer na daidaici tutiya mutu simintin gyaran kafa. Castananan 'yan simintin gyare-gyare, pressurean ƙwanƙwasa masu juzu'in juzu'in simintin gyare-gyaren juzu'ai, ƙera simintin gyare-gyare na al'ada, ɓangaren mutu da' yan wasa masu mutuwa masu zaman kansu da ƙofar da aka hatimce za a iya ƙera su. Za'a iya kerarrar 'yan simintin a tsayi da faɗi har zuwa 24 a ciki. A cikin +/- 0.0005 a cikin. Haƙuri.
ISO 9001: 2015 bokan masana'anta ta mutu magnesium, Abubuwan haɓaka sun haɗa da matsin lamba na magnesium mai matsi mai yawa har zuwa tan 200 mai ɗumi mai zafi & 3000 ton mai sanyi, ƙirar kayan aiki, gogewa, gyare-gyaren, inji, foda & zanen ruwa, cikakken QA tare da damar CMM , taro, marufi & isarwa.
ITAF16949 bokan. Servicearin Sabis ɗin Gyare Hadawa zuba jari,yashi,Kushin nauyi, Stauren ɓoye ɓoye,Siffar Centrifugal,Cast Vacuum,Dindindin Mould Gyare, .Hanyoyin iyawa sun hada da EDI, taimakon injiniya, ingantaccen samfuri da aiki na sakandare.
Fitar Masana'antu Abubuwan Nazarin sassa don: Motoci, Bikes, Jirgin sama, kayan kiɗa, Jirgin ruwa, Na'urorin hangen nesa, na'urori masu auna sigina, na'urori masu auna sigina, Na'urori, Kayan lantarki, ,unshi, Clocks, Inji, Injiniya, Kayan Kaya, Kayan Jiki, Jigs, Telecom, Haske, Kayan aikin likita, Na'urar daukar hoto, Robobi, Sassaka, kayan sauti, kayan wasanni, Kayan aiki, Kayan wasa da ƙari.
Me Zamu taimake ku yi gaba?
Je zuwa Shafin Farko Don Mutu Wasa China
→Sassan Kasuwanci-Gano abin da muka aikata.
→ Tallan kwankwasiyya Game da Ayyukan Gyare Mutuwa
By Minghe Mutu Wasa Wasa | Categories: Labarai masu Taimakawa |Material Tags: Gyare Aluminum, Zinc Gyare, Fitar Magnesium, Castan Wasanni, Bakin Karfe Cast, Fitar tagulla,Gyare Tagulla,Fitar Bidiyo,Tarihin Kamfanin,Aluminum Mutu Gyare | Comments Off